北京中仪天信科技有限公司
Here is the sturcture of H13, the tool is about 200kg weight,and it's shape like an open thin box,

to control the deformation of the tool, we used free cooling in the vacum furnace (no pressure) about 7 min in quenching,

and the temperature from 1030 down to 1000, then cooling fast.

and then we get the sturcture below.

my supervisor think the cooling rate is very low at the quenching begining, so it formed much Grain Boundary Carbieds,

but i think it,s not formed in the heat-treatment process, it's the materials fault, am i right?
200X.jpg

签到天数: 1 天

[LV.1]初来乍到

 楼主| 发表于 2009-5-4 20:51:45 | 显示全部楼层
补充张500X组织
500X.jpg
回复 顶 踩

使用道具 举报

该用户从未签到

发表于 2009-5-5 10:14:05 | 显示全部楼层
Chinese English
回复 顶 踩

使用道具 举报

签到天数: 474 天

[LV.9]以坛为家II

发表于 2009-5-5 11:02:59 | 显示全部楼层

回复 2# xianshanlushui 的帖子

Below is the microsturcture of H13, the tooling is about 200kg in weight, and it shapes like an open thin box.

To control the deformation of the tooling, we used free cooling in the vacum furnace (no pressure) for about 7 min on quenching,

and the temperature from 1030 down to 1000, then cooling fast.

and then we get the sturcture below.

my supervisor think the cooling rate is too low at the  begining of quenching, so it formed much Grain Boundary Carbieds,

but i think it's not formed in the heat-treatment process, it's the materials fault, am i right?



1. Chinese English is O,K. as long as your idea is understood. Everybody starts from somewhere.

2. It's a bit of over-etched for the 500X photo. Try a lighter eteching. Also, try different  etchants,   say. FeCl3, or else.

3. I see  few NEW (not so sure about this ) and many OLD (worm-like, inside grains) GBK films. You can see more samples of old and new gbk on my posts in my blog in Taiwan yahoo, searching with LeoMet.

[ 本帖最后由 leomet 于 2009-5-6 07:06 编辑 ]
回复 顶 踩

使用道具 举报

该用户从未签到

发表于 2009-5-20 20:02:03 | 显示全部楼层
好深奥啊,有没有中文的?
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )
Copyright © 2005-2026, rclbbs.com 苏州热协网络技术有限公司 版权所有

GMT+8, 2026-10-30 08:25 , Processed in 0.025965 second(s), 24 queries .

Powered by Discuz! X3.5

© 2001-2026 Discuz! Team.

快速回复 返回顶部 返回列表