查看: 8160|回复: 4

[求助] 有谁知道20MoCr4是什么钢材,有什么特性?

[复制链接]

该用户从未签到

发表于 2012-5-17 13:50:45 | 显示全部楼层 |阅读模式
北京中仪天信科技有限公司
有谁知道20MoCr4是什么钢材,有什么特性?十分感谢!

签到天数: 438 天

[LV.9]以坛为家II

发表于 2012-5-17 17:16:40 | 显示全部楼层
Steel 20MOCR4 (Mat.No. 1.7321, DIN 20MoCr4, AISI 8620)
Designation by Standards

Brand Name        Ravne No.        Mat. No.        DIN        EN        AISI
20MOCR4        763        1.7321        20MoCr4        20MoCr4KD        8620

Chemical Composition (in weight %)

C        Si        Mn        Cr        Mo        Ni        V        W        Others
0.20        max. 0.40        0.85        0.45        0.45        -        -        -        -

Description
One of the most popular and widely used carborizing steels available. 20MoCr4 is a hardenable chromium, molybdenum, nickel low alloy steel often used for carburizing to develop a case-hardened part. This case-hardening will result in good wear characteristics.

Applications
Gears, shafts and other applications where a hard carborized case and a tough core are desired.

Physical properties (avarage values) at ambient temperature
Modulus of elasticity [103 x N/mm2]: 210
Density [g/cm3]: 7.85

Coefficient of Linear Thermal Expansion 10-6 oC-1

20-100oC        20-200oC        20-300oC        20-400oC        20-500oC
11.1        12.1        12.7        12.9        13.5

Soft Annealing
Heat to 650-700oC, cool slowly. This will produce a maximum Brinell hardness of 207.

Heat Treatment

Treatment        Temperature        Cooling
Case hardening        880-980oC        Oil (water), hot bath 160-250oC
Carburising        880-980oC        Oil (water), hot bath 160-250oC
Direct hardening        860-900oC        Oil, hot bath 160-250oC
Core refining        860-900oC        Oil, hot bath 160-250oC
Core refining        780-820oC        Oil, hot bath 160-250oC
Tempering        150-200oC        Air

Hardenability Diagram


Click the image to enlarge the diagram.

Forging
Hot forming temperature: 1050-850oC.

Machinability
Machining is done prior to carburizing to within as close a tolerance as possible. Finish machining, after heat treatment and/or carburizing, should be at a minimum so as not to impair the hardened case of the part. Machining may be done by conventional means prior to heat treatment - after carburizing machining is usually limited to grinding.

Welding
The alloy may be welded by conventional methods, usually gas or arc welding. Preheating at 200oC is beneficial and subsequent heating after welding is recommended - consult the approved weld procedure for the method used.

Cold working
The alloy may be cold worked in the annealed condition by conventional methods. Cold working, as with machining, should be done to as close a tolerance as possible before heat treatment or carburizing.

Forms manufactured: Please see the Dimensional Sales Program.       

Disclaimer
The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Unless otherwise specified, registered trademarks are property of Metal Ravne company. Copyright 2011 by Metal Ravne. All rights reserved. Contact our Sales Office for more information.
回复 顶 踩

使用道具 举报

签到天数: 438 天

[LV.9]以坛为家II

发表于 2012-5-17 17:17:21 | 显示全部楼层
回复 顶 踩

使用道具 举报

该用户从未签到

 楼主| 发表于 2012-5-27 18:39:25 | 显示全部楼层
虽然全是英文,看着吃力但还是谢谢二位!
回复 顶 踩

使用道具 举报

该用户从未签到

发表于 2012-5-27 20:43:05 | 显示全部楼层
晕,写的看不懂,就直接告诉他是和20CrMo接近不就得了吗
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )
Copyright © 2005-2026, rclbbs.com 苏州热协网络技术有限公司 版权所有

GMT+8, 2026-11-1 03:27 , Processed in 0.023811 second(s), 21 queries .

Powered by Discuz! X3.5

© 2001-2026 Discuz! Team.

快速回复 返回顶部 返回列表