[求助] 在SA-336GrF21.CL1上堆焊Inconel600的热处理,热处理参数的选择?

[复制链接]

该用户从未签到

发表于 2009-8-25 13:10:08 | 显示全部楼层 |阅读模式
北京中仪天信科技有限公司
    我现在手头上有一个在SA-336GrF21.CL1锻件上堆焊6mm厚的Inconel600的消应力热处理,对于Inconel600这种材料我没有接触过,网上的信息比较杂乱,热处理温度有870°的也有680°的,请大虾们指导一下,这个锻件如何选择热处理参数!

该用户从未签到

发表于 2009-8-25 14:06:55 | 显示全部楼层
以下是从600的专业文献里摘出来的,稍学过英文的能看懂,大致意思好理解
In general, an annealing treatment of about 1850°F/15
min (1010°C/15 min) will produce soft material. Brief
exposure to 1900°F (1040°C) will give soft material without
producing a coarse grain structure. Grain growth does not
occur until the alloy is heated to about 1800°F (980°C). At
that temperature, the finely dispersed carbide particles in the
alloy’s microstructure, which inhibit grain growth, begin to
coalesce. Solution of the carbides begins at about 1900°F
(1040°C). Treatment for 1 to 2 hr at 2000° to 2100°F (1090°
to 1150°C) dissolves the carbides completely and results in
increased grain size. This solution treatment is beneficial in
obtaining maximum creep and rupture strength.
In general, material with a fine grain structure is
preferred because it has better corrosion resistance and
higher tensile, fatigue and impact strength. Fine-grain
material is preferred for all low-temperature applications,
most intermediate temperature applications, and those hightemperature
applications which require resistance to shockand corrosion.
Grain size is dependent on processing. Hot-rolled products
will usually have a small grain size because they are finished
at relatively low temperatures. Annealing has little effect on
the grain size of hot-rolled material. Cold-drawn or coldrolled
material, in either the cold-worked or annealed
condition, will have a small grain size. Solution treatment
will produce a coarse grain structure in either hot-worked or
cold-worked material.
The time and temperatures required for recrystallization
of cold-worked material vary widely, depending on the
amount of cold work and the specific composition. Table 25
shows times and temperatures required for recrystallization
of fine-grain sheet after various amounts of cold reduction.
你有兴趣的话,自己上www.specialmetals.com看一下
回复 顶 踩

使用道具 举报

该用户从未签到

 楼主| 发表于 2009-8-25 14:19:34 | 显示全部楼层
2# fqhhg 谢谢
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )
Copyright © 2005-2026, rclbbs.com 苏州热协网络技术有限公司 版权所有

GMT+8, 2026-10-31 03:10 , Processed in 0.022976 second(s), 21 queries .

Powered by Discuz! X3.5

© 2001-2026 Discuz! Team.

快速回复 返回顶部 返回列表